Short version of 3D printing tolerances by process: design for about ±0.3 mm on a desktop FDM part, ±0.15 mm on SLA resin and ±0.3 mm on SLS nylon, each with a percentage term on top once the feature gets longer than roughly 100 mm. Those are the numbers I put in my head before I open the CAD. They're not what the machine brochure says, and they're not what you'll get on a good day. They're what holds across ten parts from a service bureau you haven't used before.
The rest of this is about what those numbers mean for clearances, holes and fits, because that's where prototypes fail.
The numbers I design to
| Process | Typical tolerance | Sliding clearance per side | Minimum wall I trust |
|---|---|---|---|
| FDM, desktop (0.4 mm nozzle) | ±0.5%, not better than ±0.3 to 0.5 mm | 0.2 to 0.3 mm | 1.2 mm |
| FDM, industrial | ±0.15%, not better than ±0.2 mm | 0.2 mm | 1.0 mm |
| SLA resin | ±0.5%, not better than ±0.15 mm | 0.1 to 0.15 mm | 0.8 mm |
| SLS nylon (PA12) | ±0.3%, not better than ±0.3 mm | 0.3 mm | 1.0 mm |
Read the tolerance column as "whichever is larger". A 20 mm feature on SLS is ±0.3 mm, because 0.3% of 20 is only 0.06. A 250 mm housing on the same machine is ±0.75 mm, and now the percentage is in charge. Most bureaus publish figures close to these, and I'd check the one you're ordering from, since material and machine shift them a little.
Compare that with the ±0.1 mm you'd get from a machine shop without asking, or the ISO 2768 medium class on a drawing. Printed parts are three to five times looser. That isn't a defect. It just has to be designed in.
FDM: accurate in XY, moody in Z and in holes
A tuned desktop printer will hit outside dimensions in the XY plane within 0.1 to 0.2 mm on small parts, which makes people optimistic. Then the first hole comes out 0.2 to 0.4 mm undersized and the shaft won't go in.
Holes shrink for boring reasons: the nozzle lays a round path as short straight segments on the inside of the curve, the plastic pulls inward as it cools, and the first layer gets squashed outward into the opening (the elephant's foot). I oversize printed holes by 0.2 mm on diameter as a habit, 0.3 mm below about 5 mm, and if the fit matters I drill or ream it after printing. A 3.0 mm reamer costs less than the third reprint.
Z is a different story.
Height is built in layer steps, so a 10.1 mm tall boss on a 0.2 mm layer height becomes 10.0 or 10.2, never 10.1. The first layer is also squashed by an amount that depends on how the bed was levelled that morning. Any dimension I care about, I try to put in XY.
Orientation decides more than the slicer settings do. A snap hook printed standing up has layer lines across the root and breaks on the second try. Lay it flat and it works. Warping on long flat parts in ABS or nylon can lift a corner by 0.5 mm or more over 150 mm, which is outside any table.
SLA: fine detail, but check it again next week
Resin printing gives the best surface and the smallest features of the three. Embossed text 0.3 mm high is readable, 0.5 mm pins survive, and mating faces come out smooth enough to seal with a gasket. For small enclosures, lens holders and anything with fine threads modelled in, it's my first pick.
What gets underestimated is that the part isn't finished when it leaves the printer. It gets washed and UV-cured, and curing shrinks it a little more, unevenly if wall thickness varies. Thin flat walls bow. A 1.5 mm lid 120 mm long can curl by a few tenths over the following days, especially if it sits near a window. Supports leave small pips on the down-facing surface that need sanding, and a sanded surface is no longer a dimensioned surface.
So I put support faces where they don't matter, keep walls even, and add ribs to anything flat and thin. Standard resins are also brittle. A press fit that would be fine in nylon can crack a resin boss, so interference fits in SLA get a very light 0.05 mm or get replaced with adhesive.
SLS: the best functional parts, with a grainy 0.3 mm
SLS nylon needs no supports, since the powder holds the part, so internal channels, undercuts and nested assemblies are all fair game. Mechanical properties are close to isotropic. Living hinges and snap fits survive real use. For a functional prototype that'll be handled, dropped and screwed together twenty times, PA12 from SLS or MJF is what I order.
Accuracy is decent but not sharp. The surface is grainy, roughly like fine sandpaper, and that texture is itself around 0.1 mm of uncertainty on every face. Parts shrink about 3% as the powder bed cools. The bureau scales for it, but large flat panels still warp, and a 200 mm flat lid is the classic part that comes back shaped like a crisp.
For assemblies printed in one piece, leave at least 0.5 mm between moving surfaces or they'll fuse. Small holes below about 1.5 mm tend to stay packed with powder. Sliding fits between separate parts want 0.3 mm per side.
Clearances and fits that actually work
Tolerance tables are less useful than a few fit rules, so here are mine. All values are per side, between two printed parts from the same process.
- Parts that should slide freely (lids, drawers, telescoping tubes): 0.3 mm FDM, 0.15 mm SLA, 0.3 mm SLS.
- Parts that should locate snugly by hand: 0.15 mm FDM, 0.05 to 0.1 mm SLA, 0.15 mm SLS.
- Press fits: don't trust the print. Model the hole 0.1 mm under and ream, or use a crush rib 0.2 to 0.3 mm tall that deforms on assembly.
- Screws into plastic: heat-set brass inserts for FDM and SLS, with the hole sized from the insert maker's data sheet (for a common M3 insert that's close to 4.0 mm). Self-tapping screws are fine for five or six assembly cycles.
A printed part mating with a bought part is the easier case. A 608 bearing is 22.000 mm give or take a few microns, so all the variation is on your side and one test print settles it.
The mistake: tolerancing a print like a machined part
A founder once sent me a two-part handheld enclosure that had been printed three times and still wouldn't close. The CAD was clean. The lid lip and the base groove were both modelled at exactly 2.00 mm, zero clearance, because "the printer is accurate to 0.1". It was an FDM print. I opened the groove to 2.5 mm, shortened the lip by 0.3 mm so it couldn't bottom out, and the fourth print closed with a light push.
Twenty minutes of CAD. Why did it take three failed prints to get there?
Because the model was toleranced as if it were going to a mill.
The opposite mistake is just as common and costs more. Somebody puts ±0.05 mm on a printed part's drawing, the bureau either no-quotes it or quietly ignores it, and nobody knows which. If a feature truly needs 0.05, print it oversize and machine that one face or bore afterwards. It's a normal request.
And here's the counter-intuitive one: a prototype that fits perfectly can be bad news. If the design only assembles because this printer happened to run 0.2 mm small, the injection-moulded version, which will be within ±0.1 mm or better, may rattle. I'd much prefer to see the fit work in CAD with stated clearances, and then adjust the print to match, than tune the CAD until one print feels right.
What I'd actually pick for each job
For a first shape check, FDM, same day, and I don't measure anything. For small detailed parts, transparent parts or anything where surface matters, SLA. For a functional assembly that has to survive testing, SLS or MJF nylon, and I accept the grain.
Whatever the process, I print a fit coupon first when a fit matters: a 30 mm block with the critical hole, slot or snap in three clearances, say 0.1, 0.2 and 0.3 mm. It takes 15 minutes on FDM and adds very little to a bureau order. Then the real part uses the clearance that worked on that machine in that material, and the question of what the tolerance "should" be goes away.
Before the parts arrive, decide what you're going to measure. A prototype validation checklist with five critical dimensions and a pass range beats a vague impression that it "seems fine". When the design is heading for tooling later, I keep the production process in view from the start, which is most of what mechanical design and 3D modeling for a prototype involves, and the print-specific offsets live in a separate configuration so they don't leak into the production CAD.
If you've got a part that won't fit and you're not sure whether it's the design or the printer, that's a quick thing to look at. The page on functional prototyping explains how I work, and you can request a free initial DFM review of one part or assembly. You'll get short written notes on what I'd change.