For most electronics enclosures I start with ABS, move to PC or a PC/ABS blend when the part has to survive drops, heat or a clear window, pick polypropylene when it needs a living hinge or has to shrug off chemicals, and use nylon (usually glass-filled) when the part is structural rather than a cover. That covers maybe nine out of ten enclosures I've looked at.
The tenth is where the interesting decisions are. Here's how I get there.
The four materials side by side
These are typical values for unfilled, general-purpose grades. A datasheet for a specific grade will differ, sometimes a lot, so treat this table as the start of a conversation with your moulder rather than a spec.
| Property | ABS | PC | PP | PA66 (nylon) |
|---|---|---|---|---|
| Mould shrinkage | 0.4 to 0.7% | 0.5 to 0.7% | 1.5 to 2.5% | 1.0 to 2.0% |
| Heat deflection at 1.8 MPa | about 85 to 100 °C | about 125 to 140 °C | about 50 to 65 °C | about 70 to 90 °C (dry) |
| Impact | Good | Excellent | Good as copolymer, poor in the cold as homopolymer | Good once conditioned, brittle when bone dry |
| Typical wall | 1.5 to 3.0 mm | 1.2 to 3.5 mm | 1.0 to 3.0 mm | 0.8 to 2.5 mm |
| Painting and bonding | Easy | Possible, some solvents cause stress cracks | Hard without surface treatment | Moderate |
| Relative resin cost | Medium | Higher | Lowest | Higher |
Check those numbers against your grade.
Two things jump out. Shrinkage on PP is roughly three times that of ABS, which matters a lot if your enclosure has two halves that need to meet within 0.1 mm. And PP's heat deflection is low enough that a black PP housing behind a car windscreen in July is asking for trouble.
ABS: the default, and why it's the default
ABS moulds easily, holds dimensions well, takes paint, pad printing and ultrasonic welding, and has a nice surface straight out of the tool. It's forgiving. If a design has slightly uneven walls or a boss that's a bit thick, ABS will usually still give you a usable part with mild sink rather than a warped one.
Its weak points are UV (it yellows and gets brittle outdoors unless it's stabilised or painted), modest chemical resistance, and a practical ceiling of around 80 °C in service. For an indoor device with a PCB that runs warm but not hot, it's hard to beat.
A common mistake is choosing "ABS" and stopping there. There are flame-retardant grades rated UL94 V-0 at a stated thickness, high-gloss grades, high-impact grades. If there's mains voltage inside, the flame rating at your actual wall thickness is the first filter, before anything cosmetic. A V-0 rating at 3.0 mm doesn't help a 1.8 mm wall.
PC and PC/ABS: when the part takes a beating
Polycarbonate is what I reach for when a product will be dropped, stood on or run hot. It's also the obvious choice for clear windows and light pipes. It costs more, moulds hotter (melt somewhere around 280 to 320 °C), and it's notch-sensitive: a sharp internal corner that ABS would tolerate can become a crack starter in PC. Internal radii of at least half the wall thickness aren't optional here.
PC also dislikes some chemicals. Certain cleaners, sunscreen and some threadlockers cause stress cracking around screw bosses. I learned that one on a handheld device a few years ago: clean drop tests, then hairline cracks at two bosses after about a month of people actually using it. The fix was a PC/ABS blend and a slightly bigger radius at the boss root.
Cracks like that don't show up in a drop test.
That blend is often the sweet spot for handheld electronics. You keep most of PC's toughness and get better flow, easier moulding and a lower resin price.
Polypropylene: cheap, tough, and fussy about tolerances
PP is the cheapest of the four and very resistant to chemicals. It's also light (density around 0.9 g/cm³, so a part weighs roughly 15% less than the same part in ABS), and it's the only material here that makes a proper living hinge. If you're designing a battery door with an integrated hinge, or a housing that gets wiped with disinfectant ten times a day, PP deserves a serious look.
The catches are real, though. High and slightly uneven shrinkage means warpage on large flat panels. The surface is waxy, so paint and adhesives need flame or plasma treatment first. Homopolymer gets brittle in the cold, so for anything used outdoors in winter I'd specify a copolymer. And the soft, slightly greasy feel doesn't say "premium" to most people holding a consumer gadget.
Last year I reviewed a small dispenser housing drawn in PP with a 120 mm flat top and a 2.5 mm wall. It would have potato-chipped. We added two shallow ribs and a slight crown, and it stayed flat.
For a cosmetic enclosure, I'd use PP only when the hinge or the chemical resistance is the whole point.
Nylon: structural parts, not cosmetic covers
PA6 and PA66 are tough, wear-resistant and handle oil and grease well. Add 30% glass fibre and they become properly stiff, with heat deflection climbing well above 200 °C. That's why you see glass-filled nylon in brackets, clips, power tool housings and under-bonnet parts.
The thing almost everyone forgets is moisture. Nylon absorbs water from the air, and PA66 at normal room humidity can take on around 2 to 3% of its weight. That swells the part slightly and changes its stiffness and impact strength. A dry-as-moulded part is stiffer and more brittle than the same part a week later, so if your snap fits are tuned on fresh parts straight from the press, they'll behave differently in the field.
Design for the conditioned part, not the fresh one.
Glass-filled grades also shrink differently along and across the flow, so a long flat lid will try to bow. Gate location and rib layout matter far more than with ABS.
What I'd actually do for a typical enclosure
Answer three questions, in this order. What's the worst temperature the part will see, inside the box with the electronics running? Will it be dropped, and from how high? What will touch it: cleaners, skin oils, fuel, sunlight? Those three answers eliminate most options before looks come into it.
Then pick the grade, not just the family, and get its datasheet before the CAD is finished. Wall thickness, rib ratios, draft and boss design all depend on it. I'd much rather design for a known PC/ABS grade at 2.0 mm than for "some plastic" at a nominal 2.5 mm and find out at first shots that it sinks.
Finally, prototype in something close. SLS nylon is fine for checking fit, but it won't tell you how a moulded PC part cracks. If impact matters, a few machined or urethane-cast parts in a similar material are money well spent.