Gate Location: The Decision You Make Before the Toolmaker Does

Put the gate where the part is thickest, on a surface nobody looks at, so that the melt flows from thick to thin and the weld lines land where nothing is loaded. Then write that on the drawing. If you don't, the toolmaker will pick the gate that makes the tool cheapest to build, and you'll find out what that did to your part when the first shots arrive.

That's the whole argument. The details are below.

What the gate decides, apart from where the plastic goes in

The gate is a hole a millimetre or two across. It still sets most of what you'll later call "moulding defects".

It fixes where flow fronts meet, which is where weld lines form. It fixes which region fills last, which is where air gets trapped and vents are needed. It decides which sections can be packed out while the gate is still open, and which freeze off starved and sink. In glass-filled grades it sets fibre direction, and through that the direction the part warps in. And it leaves a mark: a vestige, a dimple or a blush, somewhere on your product for its whole life.

None of this shows in the CAD model. A STEP file looks identical whether the part is gated at the end, in the middle or from underneath.

Gate types and the mark each one leaves

You don't need to design the gate. You do need to know what you're agreeing to, because the gate type follows from the tool type and the tool type follows from the quote.

GateWhere it sitsMark leftTool consequence
Edge or tab gateOn the parting lineTrimmed stub, 1 to 3 mm wideSimple two-plate tool, manual or robot trim
Tunnel (submarine) gateSide wall, just below the parting lineSmall round witness, about 0.8 to 1.5 mmTwo-plate tool, shears off at ejection
Pin gateAnywhere on the top faceSmall dimple or pipThree-plate tool, more height and cost
Hot tip or valve gateAnywhere on the top faceSmall ring, nearly flush with a valve pinHot runner, no runner scrap, higher tool price
Fan or film gateAlong one edgeLong trimmed edgeFor flat parts that must stay flat

A hot runner typically adds thousands of euros to a tool, so on a small first tool most shops will offer a cold runner with an edge or tunnel gate. That's reasonable. It just means the gate will be on the perimeter, and the perimeter may be the worst place for your particular part. If tool budgets are new to you, I broke the numbers down in the mold cost estimate for small parts.

Thick to thin, and why the thick boss sinks anyway

Plastic shrinks as it cools, and the only way to make up for that is to keep pushing material in through the gate during the packing phase. That works only while there's a molten path from the gate to the section in question.

So gate into, or close to, the thickest region. If a 2 mm wall feeds a 4 mm mounting pad at the far end, the thin wall freezes first, the pad is cut off from packing pressure, and it sinks or voids no matter how the machine is set. I've had this conversation many times: the setter raises hold pressure, the gate area flashes, and the pad at the far end still has a dimple. The process isn't wrong. The gate is on the wrong end of the part. (The design-side fixes are in my article on sink marks and what causes them.)

Flow length matters too. As a rough guide, an easy-flowing PP will travel something like 250 times the wall thickness, ABS nearer 150 to 200, and PC closer to 100, all depending on grade and temperature. A 1.5 mm ABS wall therefore runs out of breath somewhere around 250 to 300 mm from the gate. If your part is longer than that, one gate at the end won't fill it, and that leads straight to the next problem.

Every extra gate buys you a weld line

People assume more gates means better filling. It does, and each added gate also adds at least one place where two cooled flow fronts meet and only partly fuse.

How weak is that? In unfilled ABS or PC a decent weld line keeps most of the base strength, typically 80% or more, and is mainly a cosmetic issue on glossy or metallic colours. In a 30% glass-filled nylon it can drop to half or less, because the fibres lie parallel to the weld and none of them cross it. That's the number to worry about.

Holes make weld lines too. The melt splits around every core pin and rejoins behind it, so each window, screw hole and vent slot has a weld on its far side, seen from the gate. Change the gate position and all of those welds rotate with it.

A couple of years ago a founder showed me first shots of a handheld housing in a glass-filled grade. The toolmaker had put a tunnel gate in the middle of one long side, which was sensible for the tool. The weld line from the display window ran straight through the root of the snap hooks on the opposite side, and the hooks cracked after a handful of assembly cycles. Moving the gate to the short end shifted the weld into plain wall. It also meant welding up and recutting an insert, which cost about two weeks.

Nobody had done anything stupid. Nobody had been told where the weld lines mustn't go.

Warp, roundness and other shape problems that start at the gate

A glass-filled part shrinks much less along the fibre direction than across it. For a PA6 with 30% glass, typical figures are around 0.3% along the flow and close to 1% across. Gate a long flat lid from one end and the fibres line up lengthwise, so the lid stays straight but narrows. Gate it in the centre and the flow is radial, the shrinkage differs between the middle and the rim, and the lid dishes like a crisp.

Round parts have their own rule. If a bore must stay round to a few hundredths of a millimetre, a single edge gate is the wrong choice, because the side opposite the gate fills last, packs least and carries a weld line. A centre gate, or three gates spaced evenly, keeps the shrinkage symmetric.

Two more that catch people out:

  • Jetting. A gate that fires into open space sprays a snake of plastic across the cavity, and it shows as a wavy mark on the surface. The gate should point at a wall or a core so the melt spreads.
  • Living hinges. The flow has to cross the hinge at right angles, in one front, with no weld on it. That usually dictates the gate before anything else does, as I explained in the piece on living hinges in polypropylene.

What I'd actually put on the drawing before the RFQ

I don't dictate a gate coordinate. The toolmaker knows their runner layout and their press better than I do, and a fixed point takes away options they may need. I mark zones instead:

Zone A, shaded, where a gate and its vestige are acceptable. Surfaces marked B, where no gate, ejector or parting-line marks are allowed. Regions marked C (snap hooks, screw bosses, seal faces, press-fit bores) where weld lines aren't permitted. A maximum vestige, for example 0.3 mm proud, or recessed in a small dimple if the surface slides against something. That's four notes and ten minutes of work on a drawing I'm making anyway.

Then one line in the RFQ: "Please confirm proposed gate type and position, with expected weld line locations, before cutting steel."

A good shop answers with a marked-up screenshot or a short fill simulation. If the answer contradicts your zones, you've learned that for the price of an email, and you can decide whether to move a feature, accept a mark or pay for a different gate. If a shop won't answer at all, that tells you something as well.

Is this overkill for a simple bracket? Probably. For a visible housing, anything glass-filled, or anything with snap fits, it's the cheapest hour in the project.

My wider list of things to settle with a moulder is in the injection molding DFM questions, and gate, weld line and vent positions are part of what I look at in an injection molding DFM review, alongside the general DFM review of walls, draft and ribs. If you have a part heading for a tool and nobody's told you where it'll be gated, you can request a free initial DFM review. We agree an NDA first, then you send the model, and I'll send back short written observations on one part or assembly.

Questions people ask

Who normally decides the gate location, the designer or the toolmaker?

The toolmaker proposes it, because it depends on the runner layout, the number of cavities and the press. The designer should still set the limits: where a gate mark is acceptable and where weld lines must not fall. Without those limits the choice is made on tool cost alone.

Can the gate be moved after the tool is made?

Sometimes. A tunnel or edge gate cut into an insert can be welded up and recut elsewhere on the parting line, which takes days to weeks. Moving from an edge gate to a top gate usually means a different tool construction, so in practice it isn't done.

How do I hide a gate mark on a cosmetic part?

Put it on a non-visible face, under a label or inside a recess, or use a tunnel gate on a side wall below the parting line. A valve gate leaves the cleanest mark on a top surface but needs a hot runner. Texture hides gate blush better than gloss.

Does a small part need a flow simulation to choose the gate?

Not always. For a simple unfilled part with even walls, experience and the thick-to-thin rule are enough. Simulation pays for itself on glass-filled materials, long thin parts, parts with many holes, and anything where weld line position affects strength.

Want a second pair of eyes on your part?

The first DFM review of one part or assembly is free: short written manufacturability notes, no simulation, no redesign. We sign an NDA first if the CAD is confidential.